It’s rare to find a component, even when searching across the entire refining and petrochemical industries, for which creep is the number one identified damage mechanism in our RBI systems. However, that is the situation which represents the vast majority of steam-methane reformer (SMR) catalyst tubes, a component which is often used right up to its metallurgical limits. Why do catalyst tubes, more so than any other common component, consistently fail by creep despite the mechanism being reasonably well understood and notionally accounted for in design?
I started writing this article with the intention of providing a short overview of catalyst tube management over their life cycles. This is an area which is familiar, having worked extensively on SMR components for the better part of the last 15 years. But because of that, words such as ‘short’ and ‘overview’ may have been ambitious. So, in the interests of readability, this article now comprises two parts:
In Part One (this part), we will cover some background to catalyst tube management and have a look at what has changed in the last few years.
In Part Two, we will use this information to look at the various aspects of catalyst tube management, starting at specification and ending at retirement.
For now, back to the original question – why do catalyst tubes still fail by creep? Well, for one thing, it is a true materials bottleneck. In other components such as most fired heaters, we can simply ‘alloy-up’, or if not, we can make it thicker. However, in catalyst tubes, there is no realistic option for alloying-up, and making it thicker is possible but undesirable from a process standpoint.
But there are other problems as well. We (as reliability engineers) at least have a predictable stress state; catalyst tubes fail due to hoop stress, i.e. pressure loading. However, temperature is another issue. Creep life is exponentially dependent on temperature, and colloquially it is halved for every 15 °C increase. As shown below, tube temperature varies in every possible dimension: tube-to-tube, axially down the length of each tube, across the wall and even slightly around the circumference. As you might expect, different profiles are expected for each of the furnace designs.
Figure 1: Tube temperature varies in every possible dimension
We monitor tube temperature, of course, which is a valuable exercise for identifying problem areas as well as trending over time, but we should almost universally expect that these numbers are an inadequate basis on which to calculate tube life. Last time we calculated corrections for background radiation reflections alone in a top-fired furnace (a desktop exercise which can be carried out using the fundamentals of radiation thermometry), correction factors of 60-70 °C were not uncommon. Even if we can trust the measurements, we must be conscious of the fact that often the critical areas are not visible, either shielded by coffin boxes or at the ends of rows where there is no line-of-sight.
Finally, there are material properties. With most engineering materials, we can look up standard properties (typically in API 530), from which we can extrapolate creep life. This approach doesn’t work for catalyst tubes, not just because there are no standard properties, but because these properties continuously change in service (we call this aging). This phenomenon has been known about for over 20 years; however, it has recently picked up steam due to some key publications.
So what has changed in the last 15 years? Well, there are some new revisions of old alloys – the result of compositional tinkering with the aim of designing the carbide distribution for optimum creep service. We want a fine distribution of carbides for creep strength, but perhaps more importantly, we need to stabilise these carbides so they remain in the microstructure, even after long periods at high temperatures.
We also have some new creep data in the published literature – among others, a PVP paper in 2023 and some excellent data out of Brazil as recently as a few months ago. Have a look at the differences between material in the as-cast condition (Stage I) and the various states of aging in the reproduced figure below. Note that this aging is not artificial; it is simply the result of service exposure over approximately 12 years.
Figure 2: Reproduced from Queiroz et al. - Aging Behavior of Nb-Modified HP Steel Tubes after Extended High-Temperature Service in Steam Reformer Furnaces: Microstructural Classification and Characterization", available https://link.springer.com/article/10.1007/s11665-026-13739-9, licensed under CC4.0'
Both are in convincing agreement with the previous work, i.e. these materials do ‘age’ naturally in service, which has implications for the creep properties originally used in design.
And finally, we have a new standard. API 561 was released as a First Edition in February this year (2026). The design requirements for catalyst tubes (we would argue) have not changed, with a lot of emphasis still put on the purchaser to approve material specifications and acceptable compositional ranges. Perhaps unexpectedly, there is a new requirement for stress rupture (creep) testing. That may help to validate manufacturers’ published data curves for virgin material (which I don’t believe were in doubt), but unfortunately does little to assist with what we care more about: the performance of continuously aging material in actual service.
So, in 2026, what does good look like? In the upcoming Part Two of this article, we will offer a few thoughts on this, through the lifecycle from design, fabrication, operation and even retirement